Dredge, spirals, dryer, magnet and electric field make ilmenite, rutile and zircon.
A mineral sands plant takes sand from an old beach or dune deposit and separates the small share of heavy minerals in it from the quartz. The heavy minerals are ilmenite, rutile, zircon and monazite. They are valuable because titanium and zirconium are used in pigments, metals and ceramics. The sand itself has little value.
The plant works in two parts. The wet plant uses water and gravity: spirals make a heavy mineral concentrate. The dry plant uses a magnetic separator and an electrostatic separator to split that concentrate into products. This overview shows the whole path, and each machine has its own lesson. Click a machine in the drawing to open it.
Everything depends on the way the minerals differ: density (heavy against light), magnetism (ilmenite against rutile and zircon) and electrical conduction (rutile against zircon). Each step uses one of these differences.
Typical features: ores of about 1 to 10 percent heavy minerals, a wet plant that discards 90 percent or more of the mass of the ore, and a dry plant that treats only the concentrate. The heavy minerals are roughly 4.2 to 5 times as dense as water, against about 2.65 for quartz: rutile about 4.2, zircon about 4.6, ilmenite about 4.7 and monazite about 5. Ilmenite is the most plentiful and is mainly used as a feedstock for titanium dioxide pigment. Rutile is nearly pure titanium dioxide, zircon is a zirconium silicate used for ceramics and foundry sand, and monazite holds rare earths and thorium. The shares of each mineral differ greatly between deposits.
Worked example, a mass balance of the plant. Assume it mines 1,000 t/h of dry sand with 5 percent heavy minerals, the slimes are 12 percent and the oversize 2 percent of the ore, and the wet plant makes 50 t/h of concentrate that is 90 percent heavy minerals.
| Quantity | Working | Result |
|---|---|---|
| Ore mined | assumed | 1,000 t/h of dry sand with 5 percent heavy minerals |
| Heavy minerals in the ore | 1,000 × 0.05 | 50 t/h |
| Slimes, 12 percent, and oversize, 2 percent | 1,000 × 0.12 and 1,000 × 0.02 | 120 t/h and 20 t/h |
| Sand fed to the spirals | 1,000 − 120 − 20 | 860 t/h |
| Concentrate at 90 percent heavy minerals | assumed 50 t/h of concentrate | 45 t/h of heavy minerals |
| Recovery of heavy minerals in the wet plant | 45 ÷ 50 | 90 percent |
| Spiral tailings | 860 − 50 | 810 t/h |
| All tailings and rejects from the wet plant | 120 + 20 + 810 | 950 t/h (950 + 50 = 1,000, so nothing is lost) |
| Concentrate leaving the wet plant at 10 percent moisture | 50 ÷ 0.90 | 55.6 t/h, which holds 5.6 t/h of water |
| Heat to evaporate that water (water only, at 2,260 kJ/kg) | 5,560 × 2,260 ÷ 3,600 | about 3,490 kW, about 3.5 MW, before the heat to warm the sand and the losses |
| Ilmenite, 60 percent of the heavy minerals | 45 × 0.60 | 27 t/h |
| Zircon, 20 percent | 45 × 0.20 | 9 t/h |
| Rutile, 10 percent | 45 × 0.10 | 4.5 t/h |
| Monazite, 2 percent | 45 × 0.02 | 0.9 t/h |
| Other grains, 8 percent | 45 × 0.08 | 3.6 t/h (27 + 9 + 4.5 + 0.9 + 3.6 = 45) |
The balance shows how little of the ore becomes product: of 1,000 t/h mined, only 45 t/h are heavy minerals and only 27 t/h of that is ilmenite. That is why the wet plant is built as cheaply as possible and runs on gravity, and the dry plant, which treats only 5 percent of the mass, can use more expensive machines.
Assumed inputs, not data from a particular plant. Ore grades, recoveries and mineral shares vary with the deposit.
Safety: a dredge pond is deep water, slurry pipes can be under pressure, the dryer is hot, the electrostatic electrode carries a dangerous high voltage, and the rare earth magnets are very strong. Dry concentrate makes dust. A concentrate that holds monazite also holds small amounts of thorium and uranium, so dust control and radiation monitoring rules can apply. This lesson shows principles, not an operating procedure.
The wet plant throws away more than 90 percent of the mass of the ore by gravity, which is cheap. The dry plant uses magnets and electricity, which cost more per tonne, so it only treats the small concentrate.
Water makes grains stick together and conduct charge over their surface. The magnet needs loose, separate grains in a thin layer, and the electrostatic stage needs grains that keep their charge.
The cut is never perfect. Some magnetic grains are only weakly held and some non-magnetic grains are carried along, so the products are cleaned again by more passes and other methods.