Nickel Processing

Two routes to nickel: sulphide ore smelted, laterite ore leached with acid under pressure.

Loading the animation…
You are watching a free lesson. A free account saves your progress and lets you mark lessons complete. Create a free account Sign in

What a nickel plant does

Nickel comes from two kinds of ore, and each has its own route. Sulphide ore holds the nickel in sulphide minerals such as pentlandite. It is concentrated by flotation, melted in a smelter and refined. Laterite ore is a soft, weathered rock in which the nickel is held in clay and iron minerals. Flotation does not work on it, so it is dissolved in hot acid under pressure and the nickel is recovered from the solution. Cobalt travels with the nickel in both routes and is separated near the end.

The animation shows both routes on one site. The back row is the sulphide route. The front row is the laterite route. Both end in a store of nickel metal. Each main piece of equipment opens its own lesson when you click it.

How it works

Both routes remove the waste step by step. The sulphide route does this with heat, and the laterite route does it with acid and water.

  1. 1Two ores. Sulphide ore is typically about 0.5 to 3 percent nickel. Laterite ore is typically about 1 to 2 percent nickel, with a little cobalt. Both are crushed and ground first (see the mineral processing plant lesson).
  2. 2Concentrate. Sulphide ore goes to flotation cells. Air bubbles lift the nickel sulphide particles as froth and leave the waste behind as tailings. A typical concentrate is about 8 to 18 percent nickel.
  3. 3Smelt and convert. The dried concentrate burns in a flash furnace that makes a molten matte and a slag. The gas goes to an acid plant. A converter then blows air through the matte to remove most of the iron and leave a richer matte.
  4. 4Refine the matte. The converter matte is cooled and ground, then leached and refined. Several refining routes are used; in the drawing it ends as nickel cathode in electrowinning cells.
  5. 5Leach the laterite. The ore slurry is heated with steam in an autoclave with sulphuric acid, at a typical 250 °C, so that the nickel and cobalt dissolve. The hot slurry is cooled in flash vessels.
  6. 6Wash and precipitate. Counter-current washing thickeners separate the solution from the solid residue, which goes to a tailings storage. Limestone and then magnesia neutralise the acid and make the nickel and cobalt come out as a mixed hydroxide.
  7. 7Separate and plate. In nickel and cobalt separation, the hydroxide is dissolved again, solvent extraction splits the cobalt from the nickel, and electrowinning plates each metal onto cathodes.

The numbers

Typical figures; every ore and plant is different. The point of the example is how much material each route has to handle. The sulphide route throws most of the rock away in flotation, so the smelter handles a small mass. The laterite route has no such step: all the ore goes through the autoclave.

Worked example. Assume 1,000 t of ore on each route. The sulphide ore is 1.0 percent nickel, flotation recovers 85 percent, the concentrate is 12 percent nickel, and smelting and refining recover 92 percent of that. The laterite ore is 1.2 percent nickel, the leach dissolves 93 percent, refining recovers 98 percent of that, and the acid use is 300 kg for each tonne of dry ore.

QuantityWorkingResult
Sulphide route: nickel in the ore1,000 × 0.01010 t
Nickel in the concentrate at 85 percent10 × 0.858.5 t
Concentrate made at 12 percent nickel8.5 ÷ 0.12about 71 t
Nickel metal at 92 percent8.5 × 0.92about 7.8 t
Laterite route: nickel in the ore1,000 × 0.01212 t
Nickel in solution at 93 percent12 × 0.93about 11.2 t
Nickel metal at 98 percent11.2 × 0.98about 10.9 t
Acid for the laterite leach1,000 × 0.30300 t

The sulphide route sends only about 71 t to the smelter, while the laterite route puts all 1,000 t through the autoclave and needs 300 t of acid to do it. That is why laterite plants need large pressure vessels, a large supply of steam and acid, and a large place to store the residue.

Assumed inputs, not data from a particular plant.

Safety: smelters handle molten metal over 1,000 °C and toxic sulphur dioxide gas, and leach plants handle hot, pressurised acid slurry and flammable solvents. Protective equipment, closed handling, gas collection and isolation of equipment are part of the design. This lesson explains the process; it is not a procedure.

What the operator watches

  • Ore grade and what is fed. Both routes depend on a steady feed of known grade.
  • Flotation recovery and concentrate grade. They set how much nickel reaches the smelter.
  • Furnace matte grade and gas. The oxygen added sets the matte grade, and the acid plant needs the gas.
  • Autoclave temperature and acid. They set how much nickel and cobalt go into solution.
  • Cobalt in the nickel product. The separation must keep it low.

Common problems

  • Nickel lost in the slag or tailings. It is metal that was mined and not sold.
  • Scale in the autoclave and its pipes. It cuts flow and heat transfer.
  • Acid use. Magnesium and other metals in the laterite use acid and raise its cost.
  • Residue storage. The washed solids are a large volume and need a safe storage.

Words you will meet

Sulphide ore
Ore in which the nickel is in sulphide minerals such as pentlandite.
Laterite
A weathered, iron-rich ore with its nickel in clay and iron minerals.
Matte
A molten mix of metal sulphides made in a smelter.
Converter
A drum in which air is blown through matte to remove iron and sulphur.
HPAL
High pressure acid leach: dissolving laterite in hot acid in an autoclave.
MHP
Mixed hydroxide precipitate: a nickel and cobalt cake from the leach plant.
Solvent extraction
Moving a metal from water into an organic liquid and back, to separate it.
Cathode
A plate of pure metal made by electrowinning.

Check your understanding

Why can sulphide ore be concentrated by flotation but laterite ore cannot?

In sulphide ore the nickel is in separate sulphide grains that bubbles can lift. In laterite the nickel is spread through clay and iron minerals, so there is nothing to float.

Where does the iron go in the sulphide route, and where in the laterite route?

In the sulphide route it goes into slag, in the furnace and the converter. In the laterite route most of it stays in the solid residue as hematite.

How much concentrate does 8.5 t of nickel make at 12 percent nickel?

8.5 ÷ 0.12 = about 71 t.

Key facts

Sulphide ore
Typically about 0.5 to 3 percent nickel, concentrated by flotation to about 8 to 18 percent.
Laterite ore
Typically about 1 to 2 percent nickel, leached in an autoclave at a typical 250 °C.
Both routes
End in nickel cathode, with cobalt separated.
Example
1,000 t of sulphide ore sends about 71 t to the smelter; 1,000 t of laterite goes all through the autoclave.
Use the animation
The animation is clickable: click the flotation cells, the flash furnace, the autoclave or its flash vessels, the washing thickeners, or the mixer-settler and cells of the separation to open their own lessons. Follow the sulphide route along the back row from the ore pile to the flotation cells, the furnace, the converter and the refining cells. Follow the laterite route along the front row from the ore pile through the autoclave and the thickeners to the precipitation tank and the separation. The numbers on the drawing match the numbered steps under How it works. Hover over any part for its name and what it does.