Silver by flotation into smelter concentrates, or by cyanide leach and zinc precipitation.
Silver is often a by-product. It comes out with lead and zinc, with copper or with gold, and in some mines it is the main metal. There are two main ways to get it out of the ore. In the first, the silver minerals are floated with the lead and zinc minerals into concentrates, which are sent to a smelter. In the second, the silver is dissolved from the ground ore with weak cyanide, caught from the solution with zinc dust in a Merrill-Crowe plant, and melted into a doré bar (silver with some gold).
The animation draws both routes on one site, so that they can be compared side by side. They share the crushers and mills at the front. A real plant normally uses the route that suits its ore, and the choice depends on the minerals the silver is in. This lesson gives the principles and typical ranges. It does not describe any particular plant. The gold version of the leach is in the gold processing plant lesson, and the copper version of flotation is in the copper processing plant lesson.
The ore moves through the plant in one line, then splits into the two routes. Steps 2 and 3 are route 1. Steps 4 to 7 are route 2.
Silver flowsheets differ a great deal from ore to ore. These are typical ranges and principles, not data from a plant.
| Item | Typical value |
|---|---|
| Grind size for flotation | typically 80 percent of the ore finer than about 75 to 150 micrometres |
| Water left in a filtered concentrate cake | typically about 8 to 12 percent |
| Dissolved oxygen after the Merrill-Crowe tower | typically below about 1 mg/L |
| Silver melting point | about 961 °C, so the furnace runs above that |
Worked example. Assume the ore holds 150 g of silver in each tonne and the plant treats 100 t/h. Route 1 sends 80 percent of the silver into a lead concentrate that is 3 percent of the feed by mass, 8 percent into a zinc concentrate that is 5 percent of the feed, and the rest to tailings. Route 2 dissolves 90 percent of the silver in the leach and precipitates 99 percent of the dissolved silver.
| Quantity | Working | Result |
|---|---|---|
| Silver in the feed | 100 × 150 g | 15,000 g/h, which is 15.0 kg/h |
| Route 1: silver in the lead concentrate | 15.0 × 0.80 | 12.0 kg/h |
| Mass of lead concentrate | 100 × 0.03 | 3 t/h |
| Silver grade of the lead concentrate | 12,000 g ÷ 3 t | 4,000 g/t, which is about 27 times the feed |
| Route 1: silver in the zinc concentrate | 15.0 × 0.08 | 1.2 kg/h, in 5 t/h, which is 240 g/t |
| Route 1: silver left in the tailings | 15.0 − 12.0 − 1.2 | 1.8 kg/h, in 92 t/h, which is about 20 g/t |
| Route 2: silver dissolved | 15.0 × 0.90 | 13.5 kg/h |
| Route 2: silver precipitated | 13.5 × 0.99 | about 13.4 kg/h |
| Route 2: share of the silver recovered | 0.90 × 0.99 | about 89 percent |
Route 1 does not make silver metal. It makes a small mass of concentrate that is rich in silver, and the smelter and refinery finish the job. Route 2 makes the silver at the mine. The two routes happen to recover about the same share here only because of the assumed figures.
Assumed inputs, not data from a particular plant.
Safety: the leach solution holds cyanide, which is highly toxic and gives off hydrogen cyanide gas if the solution turns acid. Zinc dust can burn when it is dry and dusty. Lead and zinc concentrates are toxic dusts. Smelting handles molten metal. All of them need strict handling rules. This lesson explains the process; it is not a procedure.
In many ores the silver minerals occur with the lead minerals, so they float with them.
Oxygen would use up the zinc, so more zinc would be needed and the precipitation would be poorer.
To a smelter and a refinery, which are off site. The smelter melts the concentrate and the silver follows the lead into the bullion, where refining separates it.